There are three forms of gear failure in reducers: tooth surface pitting, gear tooth breakage, and tooth thickness reduction. The first two types can be seen with the naked eye, while the third type is almost invisible - the tooth surface is still bright, with no pitting or chipping, and the teeth have become thinner. When periodic impact sounds appear and the side gap becomes significantly larger, the thinning amount often crosses the safety line early. This is the most easily misjudged type of maintenance decision-making.

This article uses the existing measuring tools in the workshop to measure the thinning into a number that can be written into the maintenance record, and then determines whether to continue using it, plan to replace it, or stop it immediately. Pitting corrosion classification and fracture judgment belong to two separate systems.

Decide on three things before taking the test

  • Take 3 to 5 tooth positions and distribute them evenly along the circumference. Repeat each position 3 times and take the average. The minimum value represents the most dangerous section, and the average value represents the overall state. Both should be recorded.

  • Fixed the same tooth position tracking, tooth top numbering. After changing the gear position, the data before and after are incomparable.

  • 20±2 ℃ or stop and cool down before testing. The linear expansion coefficient of steel is about 11.5×10⁻⁶/K. The temperature difference of 100 mm span is 10 ℃, which means the drift is 0.0115 mm. However, the threshold is usually only on the order of 0.1 mm, and the temperature alone eats up 10% of the margin.

Method 1: Public normal length, the most practical on-site

The distance read by two parallel probes of the micrometer across k teeth and stuck on the tooth surfaces on different sides is the common normal length. It only reflects the tooth thickness, and the effects of tooth direction and tooth shape errors are basically offset. It can be measured without unpacking and with an observation window. When α=20°, the number of span teeth k = z/9 + 0.5 (rounded), standard spur gear W = m·cosα·[π(k−0.5) + z·invα] , inv20° = 0.014904.

Calculation example: m=5, z=30, k=3.83, take 4, W = 5×0.9397×[π×3.5 + 30×0.014904] ≈ 53.76 mm . The common normal shortens after wear, and the conversion must be divided by the cosine of the pressure angle: Δs = ΔW / cosα , which is approximately 1.064 times at 20°. Some data write it as 1.414 times, which is the relationship of 45° pressure angle. Applying it to a 20° gear will overestimate the wear by 30%. The actual measurement of the same example is 53.66 mm, Δs=0.106 mm, accounting for 1.36% of the standard tooth thickness πm/2 = 7.854 mm, which is a normal running-in.

Helical gears can only measure the normal direction, and the tooth width must satisfy b > W·sinβb. Otherwise, the probe cannot catch the tooth surface, so the measuring cylinder method must be used instead.

Method 2: Tooth thickness caliper, fast but one level lower in accuracy

Use a caliper to measure the thickness of the fixed string teeth. Use a vertical ruler to measure the height of the tooth top first, and then a horizontal ruler to clamp the tooth surface. sc = πm/2·cos²α ≈ 1.387m (m=5, about 6.93 mm). It can be operated with one hand and is not limited by tooth width. It is suitable for reducer maintenance and inspection of coarse screening; however, the positioning depends on the tooth top circle. After the tooth top is worn, the reading will be too large, and the accurate rejection will still return to the public normal line.

How to choose among the four methods

method

Accuracy

No unboxing

Applicability and limitations

common normal micrometer

0.01 mm

There is an observation window available

Straight teeth and helical teeth with sufficient tooth width; main basis for judgment

Tooth thickness caliper

0.02mm

Can

Coarse screening; relies on intact addendum circle

Column method (M value)

0.01 mm

Need to open the lid

Internal teeth, small module, narrow tooth width

Three-dimensional coordinate/optical scanning

0.005~0.01mm

否

Overhaul damage determination and dispute arbitration

The invalidation threshold is a table, not a line

'Replace after 10% wear' is too rough. The allowable thinning amount is related to the tooth surface hardness and impact degree: after carburizing and quenching of the hard tooth surface reducer, the margin before the hardened layer is worn through is very small; thinning under impact conditions will quickly amplify the tooth root stress, and the threshold must be tightened.

Working conditions and tooth surface

Allow tooth thickness to be reduced

Dispose

Stable and light load (machine tool feeding, packaging line)

5%~8%

Continue to use and shorten oil changes

Medium impact (conveying, mixing)

8%~10%

Included in planned maintenance

Heavy load impact (breaking, lifting)

3%~5%

Spare parts are replaced as soon as they are available

Soft tooth surface gear

15%~20%

Replace in pairs

Hard tooth surface and hardened layer see the interface

5%, absolute value ≤ 0.20 mm

Stop immediately

Why is the threshold so low? The tooth root bending stress is approximately inversely proportional to the square of the tooth thickness: if the thickness is reduced by 10%, the stress will increase by approximately 23%, and if the thickness is reduced by 15%, the stress will increase by approximately 38%. The gears are designed according to fatigue life, the stress increases by 30%, and the remaining life drops to less than one third.

Determine the remaining life from the thinning amount

The data at two time points can be used to calculate the rate and extrapolate: R = Δs cumulative ÷ operating hours ,remaining hours = (s limit − s current) ÷ R . A certain induced draft fan reducer is thinned by 9.3% after running for 42 000 h, and the annual operation is 6 000 h. R = 0.93%/10 000 h. According to the 15% limit, the remaining time is about 6 100 h, that is, one year. Wear accumulates linearly, and the jump only occurs after lubrication fails or foreign matter enters. When the slope becomes steeper, check the oil first.

The three most common misjudgments

One is to regard the increase in side clearance as wear. The backlash is determined by the tooth thickness, center distance and bearing clearance. The running of the outer ring of the bearing also increases the backlash. At this time, changing the gear is equivalent to replacing it in vain. The order must be to measure the clearance first and then the common normal. The second is to only measure one tooth and draw the conclusion: the eccentric load wear is concentrated at one end of the tooth width, and a single point may read 2% or 12%. The same is true for the pin tooth sleeve of the cycloidal pinwheel reducer , and points must be taken throughout the circle. The third is to ignore circumstantial evidence of efficiency and temperature rise: the tooth surface Ra rises from 0.4 μm to 1.6 μm, the transmission efficiency of the reducer drops by 1 to 2 percentage points, and the oil pool temperature rises by 5 to 8 K, all of which occur earlier than the dimensional deviation.

Conclusion: Make the wear amount into a curve

Measuring tooth thickness is not difficult. What is difficult is repeating the measurement at the same tooth position, the same temperature, and the same micrometer. As long as there is a thinning table arranged by date in the maintenance record, the timing of overhaul is no longer determined by 'something doesn't sound right'; data can also be used to explain whether the reducer parts should be replaced in pairs - if the thinning amount of the same pair of meshing gears differs by more than 2 percentage points, the entire set should be replaced. Replacing one gear alone will accelerate failure due to tooth shape mismatch.

Hangzhou Weigao Transmission provides a full range of hardened tooth surfaces, worm gears, cycloid pinwheels and gear reduction motors. Parameters can be compared and replaced according to SEW, NORD and other brand models Selection. Send us the module, number of teeth, original common normal and actual measured values, and we can help calculate the thinning rate for free, determine whether to enter the replacement window, and provide a checklist of installation dimensions for the replacement model.

FEEDBACK

Gearbox Shaft Seal Selection: Lip, Labyrinth or Cassette for Wet Duty

How to check the bearing capacity of reducer gears: Calculation examples of contact stress and tooth root bending stress - Hangzhou Weigao Transmission

What methods can be used to avoid failure of the internal gear transmission system of CJY reducer?

What impact will a gear transmission system failure have on the CJY reducer?

Gearbox Market 2027: Retrofit Demand in Southeast Asian Palm Oil Mills